Quick answer: To make encaustic paint, melt about 8 parts beeswax with 1 part damar resin (by weight) at roughly 200°F, strain out the resin’s debris to create encaustic medium, then stir in dry pigment, starting at about 1 part pigment to 10 parts medium by volume. Pour the mixture into small tins or a muffin pan to cool into cakes. Adjust the ratios for a harder or softer paint and always test on a scrap panel.

Store-bought encaustic paint is convenient but expensive, and you are limited to the colors a brand happens to sell. Learning how to make encaustic paint yourself lets you mix exact colors, control translucency and produce large batches of medium for a fraction of the cost.

The process is closer to cooking than chemistry. You melt two ingredients, filter them, add color and pour. What makes the difference between a good batch and a frustrating one is the ratio, the temperature and how carefully you incorporate the pigment.

What You Need

Ingredients

  • Beeswax: Filtered, ideally cosmetic or art grade. Bleached white beeswax gives truer color mixing. Natural yellow beeswax adds a warm cast, which some painters like.
  • Damar resin crystals: A natural tree resin that hardens the wax, lets you buff the surface and raises the melting point.
  • Dry pigments: Artist-grade powdered pigments. Alternatively, oil paint sticks or tube oil paint can be used in small amounts (see below).

Equipment

  • A heated palette, electric skillet or hot plate with temperature control
  • A dedicated metal pot or large tin for melting medium (never return it to food use)
  • A kitchen scale
  • Fine metal mesh strainer, cheesecloth or a paint strainer
  • Small metal tins, a silicone or metal muffin pan or candy molds
  • Metal spoons or palette knives for stirring
  • A thermometer
  • A dust mask or respirator and nitrile gloves for handling dry pigment
  • Good ventilation (an exhaust fan near your heat source)

A heated palette with even, adjustable heat makes both the melting and the painting steps easier. If you are still choosing one, our breakdown of the best wax palettes for encaustic work explains which features matter for mixing your own paint.

Choosing Your Wax-to-Resin Ratio

Damar changes how the paint behaves. More resin means a harder, glossier, more brittle film. Less resin means softer wax that buffs to a duller sheen and may be slightly tacky in warm rooms.

Wax : damar (by weight)HardnessBuffingWhen to use it
10 : 1SofterSatinCooler climates, softer feel, more flexible on paper
8 : 1BalancedGood sheenThe standard starting point for most artists
6 : 1HarderHigher glossHot climates, more scratch resistance
4 : 1 or more resinBrittleVery glossyGenerally not recommended; can crack

If you are new to this, start at 8 to 1. For example, 16 ounces of beeswax with 2 ounces of damar yields roughly 18 ounces of medium.

How to Make Encaustic Paint: Step-by-Step

Part 1: Make the Encaustic Medium

  1. Set up ventilation. Open a window and run an exhaust fan near your work area before turning on any heat.
  2. Weigh the ingredients. Measure beeswax and damar separately on the scale.
  3. Melt the wax. Put the beeswax in your dedicated pot and heat to about 200°F. Beeswax melts at around 145°F, but the extra heat helps the resin dissolve.
  4. Prepare the damar. Crush large crystals into smaller pieces by wrapping them in a cloth and tapping with a hammer. Smaller pieces dissolve faster.
  5. Add the damar. Stir the crystals into the molten wax. They take time to dissolve, often 30 minutes to a few hours depending on crystal size and temperature. Stir occasionally.
  6. Keep it below about 220°F. If the wax smokes, lower the heat. Overheating darkens the medium and creates more fumes.
  7. Strain. Damar crystals contain bits of bark and grit. Pour the melted medium through fine mesh or cheesecloth into a clean container.
  8. Pour into molds. Pour the clear medium into a muffin pan or tins and let it cool. Pop out the cakes once fully set.

Part 2: Add Pigment

  1. Melt a portion of medium. Place a cake of medium in a small tin on your palette.
  2. Put on a mask and gloves. Dry pigment is a fine dust; avoid inhaling it.
  3. Add pigment gradually. Start with about 1 part pigment to 10 parts medium by volume. Sprinkle it in rather than dumping it, which creates clumps.
  4. Stir thoroughly. Mix with a metal spoon or palette knife for several minutes, pressing clumps against the side of the tin.
  5. Test the color. Brush a stroke onto a scrap panel or index card, let it cool and fuse. Melted wax looks darker and more saturated than the cooled color.
  6. Adjust. Add more pigment for opacity and intensity, or more medium for translucency.
  7. Pour into tins or molds. Label each cake with the pigment name and ratio.

Pigment Loading: How Much Is Too Much?

Every pigment has a different tinting strength, so there is no single correct amount. Strong modern pigments like phthalo blue need very little. Earth colors and some whites need more.

Pigment typeTypical starting loadNotes
Phthalo blue/green, quinacridonesVery low, often under 5 percentExtremely strong; a little goes far
Cadmiums, cobaltsAbout 10 to 15 percentHandle with extra care; toxic as dust
Earth colors (ochres, siennas, umbers)About 10 to 20 percentMix easily and are inexpensive
Titanium whiteAbout 15 to 25 percentNeeded for opaque whites
Iridescent or mica powdersAbout 5 to 10 percentGood for shimmer glazes

These percentages are approximate starting points by volume. Too much pigment can make paint chalky, dull and weak, because there is not enough wax to bind the particles. If a cooled stroke rubs off as powder, add more medium.

Using Oil Paint or Oil Sticks Instead of Dry Pigment

If you already own oil paints, they can tint encaustic medium. This avoids handling dry pigment but introduces oil, which softens wax and slows hardening.

  • Blot tube paint first. Squeeze oil paint onto paper and let it sit for a few hours so some oil soaks out.
  • Keep it to a small proportion, commonly around 10 to 20 percent of the mix at most.
  • Oil sticks contain wax already and blend into medium easily.
  • Test for tackiness. If a cooled stroke stays soft or sticky after a day, the mix contains too much oil.

How to Make a Wax Palette of Colors

Once you know how to make one color, building a full set follows naturally. A practical starter set is:

  • Titanium white
  • Yellow ochre
  • A warm yellow and a cool yellow
  • A warm red and a cool red
  • Ultramarine blue and phthalo blue
  • Burnt umber or burnt sienna
  • Black (or mix from umber and blue)
  • Plenty of clear medium

Mixing a limited color palette into secondary colors on your heated palette teaches color relationships quickly and keeps your paintings harmonious. Make medium in large batches; you will use far more of it than any single color.

Cost and Batch Planning

The main reason many painters switch to homemade paint is volume. Prepared encaustic colors are sold in small cakes, and clear medium is used so heavily that buying it ready-made adds up quickly. Raw beeswax and damar crystals cost far less per pound than finished medium, and a single pound of dry pigment can tint a large quantity of paint because only a fraction of each cake is pigment.

Plan batches around how you work:

  • Medium: Make the largest batches you can store, for example 2 to 5 pounds at a time. You will use it for priming, glazing and thinning.
  • White: Make a generous batch, since most mixtures and tints rely on it.
  • Strong colors: Make small batches of intense pigments like phthalos, then mix them into medium as needed.
  • Test colors: Make tiny batches in single tins until you know you like a pigment.

Keep a simple log of each recipe: pigment name, amount of medium, amount of pigment and the date. When you love a color, you can repeat it exactly.

Grinding Pigment for Smoother Paint

Some pigments disperse easily in wax; others form stubborn clumps. Professional encaustic makers grind pigment into the wax on a heated surface, much like mulling oil paint. You can do a simple version at home: put a small pile of pigment on a heated metal plate or palette, add a little molten medium, and work it with a palette knife or glass muller in circular motions until smooth. Then stir that concentrated paste into a larger tin of medium. The extra step produces more even color and fewer speckles, especially with organic pigments.

Variations and Additives

  • Microcrystalline wax: A petroleum-derived wax sometimes used instead of beeswax. It is softer and more flexible. Some artists blend a portion with beeswax for paper work.
  • Carnauba wax: A very hard plant wax. Small additions raise hardness and melting point but can make paint brittle.
  • Translucent glaze medium: Medium with just a pinch of pigment for veils of color.
  • Textured paint: Some painters stir in fine marble dust to stiffen paint for sculptural effects.

Testing a New Batch Before You Paint

Before using a fresh batch on a real piece, run a quick test. Brush three strokes onto a primed scrap panel: one of pure color, one mixed about half and half with medium, and one heavily diluted glaze. Fuse all three, let them cool for an hour, then check each against a few questions. Does the color look as you expected once cool? Does a fingernail leave a deep scratch (too soft) or does the stroke chip (too hard)? Does buffing with a soft cloth produce a gentle sheen? Answers to these tell you whether to adjust pigment, resin or oil before committing.

Storing Homemade Encaustic Paint

Cooled cakes keep indefinitely. Store them in labeled containers away from heat and direct sun. Wrapping each cake in wax paper prevents dust from settling. When you need a color, drop a cake in a tin on your palette; wax can be remelted many times, although repeated overheating may darken it.

Troubleshooting Homemade Encaustic Paint

ProblemLikely causeFix
Grainy or speckled colorClumped pigmentStir longer; grind pigment with a little medium on a hot surface first
Chalky or powdery strokesToo much pigmentAdd more medium
Paint cracks on the panelToo much resin or a flexible supportUse less damar; switch to a rigid panel
Sticky surface after coolingToo much oil or too little resinReduce oil paint; increase damar slightly
Medium looks brownOverheating or natural beeswaxLower temperature; use bleached beeswax
Debris in mediumUnstrained damarStrain through finer mesh

Safety Reminders

  • Never melt wax over an open flame on a stove; use controlled electric heat.
  • Keep temperatures below the smoking point.
  • Ventilate the room throughout melting and painting.
  • Wear a dust mask and gloves when handling powdered pigments.
  • Keep a fire extinguisher nearby and never use water on hot wax.
  • Keep all encaustic equipment separate from food utensils.

FAQs

What is the ratio of beeswax to damar resin for encaustic?

The most common ratio is about 8 parts beeswax to 1 part damar resin by weight. Many artists adjust between roughly 6 to 1 and 10 to 1 depending on climate and preferred hardness.

Can you make encaustic paint with crayons?

Crayons are paraffin with low-quality pigment. They melt, but the paint is soft and colors may fade. They are fine for casual experiments or kids’ projects, but not for lasting artwork.

Do you need damar resin to make encaustic paint?

Plain beeswax with pigment works, but it stays softer, is easier to scratch and does not buff to the same sheen. Damar improves durability and surface quality.

Can you use wax paper for a wet palette or in encaustic?

Wax paper is not a substitute for the membrane in an acrylic wet palette, but in encaustic it is handy for wrapping cakes of paint and covering finished paintings during storage.

Can you add acrylic paint to encaustic wax?

No. Acrylic paint contains water and does not mix with molten wax. Use dry pigment, oil sticks or small amounts of blotted oil paint.

How long does homemade encaustic paint last?

Cooled encaustic paint keeps essentially indefinitely when stored away from heat and dust. Wax can be remelted many times.

Next Step

Making your own encaustic paint comes down to a reliable ratio, controlled heat and careful mixing. Start with an 8 to 1 medium, a few earth pigments and white, then expand your color set as you learn how each pigment behaves. Even heating is what keeps homemade paint consistent, so see our guide to choosing a heated palette for encaustic paint before scaling up your batches.

Facebook
Pinterest
Twitter
LinkedIn
Reddit
Telegram
Picture of Md Jomiruddin Sobuj

Md Jomiruddin Sobuj

Md Jomiruddin Sobuj is the founder and editor of PaintingProGuide. He comes to art supplies from digital publishing rather than from a studio, and the site reflects that: every guide here is built from manufacturer specifications, product documentation and the patterns that show up across hundreds of real user reviews — the details that predict how a brush, a paint or an easel actually behaves once you are using it. He writes or edits every article on the site and is accountable for what each one says, including telling you when a product is wrong for you. Corrections and questions are genuinely welcome at contact@paintingproguide.com.

Related Post

Choosing the best palette for upcycled art helps mix and apply paints

The correct thumb-and-forearm grip for a painting palette, plus balance, paint layout

Choosing the best palette for advertising illustration can boost your design’s impact.

Choosing the best palette for social art boosts creativity and makes painting

Leave a Reply

Your email address will not be published. Required fields are marked *

Picture of Paintingproguide

Paintingproguide

Painting

Welcome to PaintingProGuide, your ultimate resource for all things related to painting! Whether you’re a seasoned artist or just starting out, our mission is to inspire, educate, and empower you to create your best work. We believe that everyone has the potential to be an artist, and our goal is to help you unlock your creativity and achieve your artistic dreams.

Recent Posts